الکترود جیکا TEMPO B 70 S

TS EN ISO 18275-A

E 55 6 2NiMo B T 4 2 H5

EN ISO 18275-A

E 55 6 2NiMo B T 4 2 H5

AWS A5.5

E9018-G H4

Chemical Composition of Weld Metal % (Typical)

C

Si

Mn

Ni

Mo

0,07

0,2

0,6

2,4

0,4

Typical Base Material Grades
  • S380N-S500N, S355NH-S460NH, S380NL-500NL
  • Fine grained, high alloyed steels and steel castings
  • API 5L: X52, X56, X60, X65, X70
Mechanical Properties

Yield Strength (N/mm²)

Tensile Strength (N/mm²)

Impact Strength (ISO-V/-60°C)

Elongation ((Lo=5do) (%))

Heat Treatment

min. 550

620-780

min 47 J

min. 18

560-600°C / 1 h / furnace down to 300°C / cooling at (air)

Features and Applications
  • Suitability for use in welding of high-strength , fine-grained steels
  • High ductility and high resistance to cracking obtained in welding fine-grained steels
  • Suitability for use in welding of materials with service temperatures between -60°C and +350°C
  • Welding of the all-weld metal test assembly shall be executed in the temperature range 120 °C to 175 °C with the exception of the first layer which may be welded without preheat.
  • Re-drying: 300-350°C / min. 2h
Current Type
  • DC(+)

 

Operating Data

Product Code

Diametré x Length (mm)

Diameter x Length (inch)

Welding Current (A)

Weight g / 100 pcs

3010100570

ø2,5 x 350

ø3/32 x 14

80 - 110

2320

3010100573

ø3,2 x 350

ø1/8 x 14

100 - 140

3670

3010100576

ø4,0 x 450

ø5/32 x 18

130 - 190

6790

3010100579

ø5,0 x 450

ø3/16 x 18

190 - 240

10130